HV cable materials glossary: XLPE, CCV, Um and more

· Basics

This glossary covers the terms used on HV cable compound data sheets and in the cable specifications that call for them. Each entry gives a plain definition first, then what the data sheets or standards say. Grade facts come from the current (2026) Borealis data sheets for the Borlink™ grades we supply, and voltage and test terms from the IEC standards; where neither defines a term, we name the specification, patent, conference paper or equipment maker that uses it. Property values quoted from the Borealis data sheets’ property tables, such as resistivity, are typical values, which Borealis says should not be used for specification work.

Materials

XLPE

Cross-linked polyethylene, the insulation layer of a modern power cable: a natural (uncoloured) polyethylene compound that cross-links after extrusion, in the vulcanizing tube, into a tough, heat-resistant dielectric.

Each of the four Borlink™ insulation grades we supply, LE4244S, LS4201S, LE4244EHV and LS4201EHV, is described on its data sheet as a ready-to-use crosslinkable natural polyethylene (XLPE) compound. The sheets give the melt flow rate without peroxide, and measure properties such as tensile strength and hot set on crosslinked specimens.

Peroxide crosslinking leaves by-products that HV cable cores are degassed to reduce (see degassing). Grades and properties: XLPE insulation; how the four grades differ: Borlink™ LE4244S vs LS4201S.

Superclean

The word the Borlink insulation data sheets use for cable insulation made from a compound with an assured cleanliness level. They publish no cleanliness figure.

All four current sheets call cleanliness a critical parameter in the grade’s intended application, and say the level is assured through the Borealis quality management system. The 2026 editions add that it is “verified in several process steps against stringent specifications using Borealis proprietary analysis techniques”.

Cleanliness also has to survive handling. The same sheets call careful, very clean handling essential to a good and reliable cable, and say material handling should be conducted in closed systems and clean-room conditions (the LE4244EHV sheet says “preferably”). Stock we hold stays in its sealed original packaging, unopened until dispatch: see our warehouse and why superclean insulation matters.

Greece’s Independent Power Transmission Operator (IPTO) also uses the word: its specification TD-102/3 requires the insulation of its 400 kV cables to be a “super clean” extruded XLPE layer. The Borlink data sheets do not reference IPTO or TD-102/3.

Supercure

A Borealis technology name. LS4201S and LS4201EHV are described on their data sheets as compounds “based on Supercure technology”, but neither sheet explains what the technology is, and the LE4244 sheets do not mention it. Both LS4201 sheets separately list very good electrical performance, excellent scorch resistance enabling long production runs, and high productivity due to a reduced degassing burden, without saying which of these come from Supercure. See scorch, degassing and how the four insulation grades compare.

Semiconductive screen

One of the two carbon-filled layers around the XLPE insulation of an HV cable: the conductor screen over the conductor, and the insulation screen over the outside of the insulation. Both even out the electric field. IPTO’s TD-102/3 calls them the semi-conducting layers for the conductor and for the insulation.

The screen grades we supply are crosslinkable black polyethylene compounds: LE0592S for the conductor screen and bonded insulation screen of HV AC cables, LE0500 for the same layers in EHV AC cables, and LE0550DC for the conductor screen and insulation screen of HVDC cables.

The resistivity gap to the insulation is wide. The three screen sheets give a typical DC volume resistivity below 100 Ω·cm at 23 °C and below 1000 Ω·cm at 90 °C; the four insulation sheets give above 10 PΩ·cm at 23 °C. More on the grades: semiconductive screens and the layers of an HV cable.

Bonded and strippable screens

A bonded insulation screen is fully adhered to the insulation; a strippable one is peeled off for jointing. The Borlink data sheets use both words for cable constructions without defining them. Each screen sheet states its use like this:

  • LE0592S (HV AC): conductor and insulation screen for bonded cable constructions, and conductor screen for strippable cable constructions.
  • LE0500 (EHV AC): conductor screen and bonded insulation screen.
  • LE0550DC (HVDC): conductor screen and insulation screen of HVDC power cables; its sheet uses neither word.

None of the eight grades we supply is described as a strippable insulation screen. See semiconductive screens.

Supersmooth

Borealis’s description of LE0500 and LE0550DC, both called supersmooth crosslinkable black polyethylene compounds. Their sheets attribute a superior smoothness of the semiconductive screen to the excellent distribution of carbon black and additives. The HV screen grade LE0592S is not called supersmooth; its sheet says the same kind of distribution results in a very smooth screen. None of the sheets gives a smoothness measurement.

HVDC screen compound

A semiconductive compound for the conductor screen and insulation screen of HVDC power cables. LE0550DC is the HVDC grade we supply: its data sheet (Ed.1, April 2026) calls it supersmooth and intended for the semiconductive screens of XLPE HVDC cables. Under Specifications it lists IEC 62895 (test methods and requirements for HVDC land cable systems with extruded insulation) and CIGRE Technical Brochure 852 (Working Group B1.62’s 2021 recommendations for testing extruded DC cable systems). Both documents set their own voltage scopes; the LE0550DC sheet itself states no voltage rating. We supply no HVDC insulation grade.

Foamed dielectric

Dielectric insulation that contains closed foam cells. Teflon™ FFR 770 is a fluoroplastic resin with a foam nucleating package, foam-extruded with nitrogen gas injection. Chemours says foaming reduces the resin’s dielectric constant, and positions FFR 770 for foamed primary dielectric insulation of twisted-pair and miniature coaxial cables.

According to the sheet, a typical cable core has 20–65 % void content, in closed cells from 0.018 to 0.033 mm (0.0007–0.0013 in) in diameter; achievable void content varies with wall thickness and processing conditions. The sheet’s typical property table gives a dielectric constant of 2.04 at 1 kHz, 1 MHz and 1 GHz, without saying whether this value is measured on solid or foamed material. Background: foam extrusion with FFR 770 and power-cable vs signal-cable materials.

Processing

Triple extrusion

Extruding the conductor screen, insulation and insulation screen in a single pass and cross-linking them together. IPTO’s TD-102/3 makes both semi-conducting layers compulsory and says they “must be produced together during production with the triple extrusion method”.

The Borlink data sheets do not mention triple extrusion, and each says its information relates to the product when not used with other materials. Choosing and qualifying the screen and insulation combination is the cable maker’s job. Related: semiconductive screen, 500 kV cables and the layers of an HV cable.

CCV

Catenary continuous vulcanizing: a production line that insulates and vulcanizes (cross-links) a power cable core in one continuous run. The cable-line maker Maillefer describes its CCV lines as serving power cables from medium to extra high voltage. For insulation droop on these lines, see sagging.

The LE4244S and LE4244EHV data sheets say each grade is specially designed for extrusion on horizontal lines and for cables with thick insulation walls extruded on CCV lines. The LS4201 sheets name no line type.

VCV

Vertical continuous vulcanizing: the vertical form of a continuous insulating and vulcanizing line. Maillefer describes these lines as serving high and extra high voltage cable, and Borealis’s patent US 11708431 B2 uses the abbreviation VCV. None of the Borlink data sheets we supply mentions vertical lines.

Sagging

Downward movement of the insulation while it is still molten, which leaves the cable core eccentric. A Borealis patent, US 11708431 B2 (“Polymer composition comprising a polyethylene”), describes two forms. On horizontal continuous vulcanization lines, the conductor may sink within the insulation if a polymer with too high a melt flow rate (MFR2) is used. On CCV lines, soft molten insulation may drop off the conductor and shift the insulation layer downward. The patent says improved sagging resistance is needed for big cable constructions and for production on catenary and horizontal cable lines. It names no Borlink grade.

Maillefer describes a related effect on CCV lines: when the viscosity of the material near the conductor falls, as with a rapid temperature rise, the insulation droops and ends up off-centre.

Of the grades we supply, the LE4244S and LE4244EHV data sheets state very low sagging properties. They give no sag measurement, and the LS4201 sheets do not mention sagging. More: Borlink™ LE4244S vs LS4201S.

Scorch

Cross-linking that starts too early, in the extruder. Borealis’s patent application EP 2468813 A1 (“Scorch resistant polyethylene composition”) explains that it happens if a significant amount of peroxide already decomposes in the extruder, and that the so-called scorch means “inhomogeneity, surface unevenness and possibly discoloration in the different layers of the resultant cable”. The application names no Borlink grade.

The LS4201S and LS4201EHV data sheets list excellent scorch resistance enabling long production runs. Neither current sheet gives a scorch-time value.

Degassing

A process that reduces the concentration of crosslinking by-products in a cable core. A Jicable’11 paper (E.7.1.3) by Ericsson AB and Borealis AB authors says the cores of crosslinked HV cables have to be degassed for both technical and safety reasons:

  • Methane, formed during peroxide crosslinking, has to be removed to eliminate the risk of fire or explosion during handling and installation.
  • The polar by-products, mainly acetophenone and cumyl alcohol, influence electrical properties such as dissipation factor and space charge accumulation.

The LS4201S and LS4201EHV data sheets say each grade is specially designed for high productivity due to a reduced degassing burden. They do not quantify the reduction or give degassing conditions.

Pre-drying

Drying a compound before extrusion. The three Borlink semiconductive data sheets, LE0592S, LE0500 and LE0550DC, give a typical drying temperature of 60 °C, with a footnote of 4 h with dehumidified air, and the LE0592S sheet recommends drying before extrusion. The four insulation data sheets contain no drying setting. More in our storage and pre-drying guide.

Storage and handling

Shelf life

The storage period a data sheet gives for a grade, counted from the production date, for material in unopened original packages under dry and clean conditions within a stated temperature window:

Grade Shelf life Storage temperature Higher-temperature allowance
LE4244S, LE4244EHV 12 months 10–35 °C (50–95 °F) Up to 40 °C (104 °F) for up to 6 months
LS4201S 24 months 5–35 °C (41–95 °F) Up to 40 °C (104 °F) for up to 6 months
LS4201EHV Not stated (Ed.3 has no storage section) — —
LE0592S, LE0500, LE0550DC 18 months 10–30 °C (50–85 °F) None stated

The 40 °C allowance has the same package and storage conditions. The sheets add that extreme conditions influence the general quality and performance of the material. The LE4244S, LS4201S and LE4244EHV sheets also ask for the material to be conditioned indoors, in the production room, to reach ambient temperature before use. For Teflon™ FFR 770, Chemours states that the resin’s properties are not affected by storage time, and that ambient storage should avoid airborne contamination and water condensation on resin removed from its containers.

We hold stock in sealed original packaging in a dry, clean, climate-controlled warehouse in Shanghai: see our warehouse and the storage guide.

FIFO

First In – First Out: stock rotation that uses the oldest material first. Six of the seven Borlink data sheets recommend proper stock rotation on this principle and refer to the safety data sheet (SDS) or product safety information sheet (PSIS) for more information on storage; LS4201EHV Ed.3 has no storage section. In our Shanghai warehouse, first-in-first-out stock rotation protects shelf life, and every lot is traceable to its production batch and COA.

Voltage and tests

Um

The highest system voltage: in IEC 60183:2015 (3.1.3), the highest r.m.s. power-frequency voltage between conductors that the cables and accessories are designed for. It is the highest voltage sustained in normal operation anywhere in the system, leaving out temporary variations from faults or the sudden loss of large loads.

Cables are designated U0/U (Um), where U0 is the rated voltage between conductor and screen or sheath and U the rated voltage between conductors (3.1), and Um should be chosen not less than the highest voltage of the three-phase system (5.3). IPTO’s 400 kV cables, for example, are rated Uo/U(Um) = 230/400(420) kV.

The term in IEC 60038 is “highest voltage for equipment” (3.9): equipment may only be used on systems whose highest system voltage does not exceed it. Its Table 4 pairs nominal system voltages of 220 and 230 kV with a highest voltage for equipment of 245 kV. The Borlink data sheets use the same pairing: their HV grades are for AC cables rated up to 230 kV (Um = 245 kV), the values being voltages between phases as defined in IEC 60183. Voltage classes: 110 kV · 220 kV · 330 kV · 500 kV.

HV and EHV

High voltage and extra-high voltage. Sources draw the line between them in different places, so check which split a document uses.

The Borlink data sheets split their AC grades at 230 kV. The HV grades, LE4244S, LS4201S and LE0592S, are for AC cables with rated voltages up to 230 kV (Um = 245 kV). The EHV grades, LE4244EHV, LS4201EHV and LE0500, are for rated voltages above 230 kV.

A NEETRAC paper at Jicable’19 on North American service experience grouped HV as 69–150 kV and EHV as 230–400 kV, groupings it describes as based on IEC standards, and the IEC cable test standards split at 150 kV (see IEC 60840 and IEC 62067). A 220 or 230 kV cable therefore falls under the scope of IEC 62067 but within the stated application of the HV grades: see 220 kV, 330 kV and choosing the HV or EHV version. Where a system rated 230 kV or below has a Um above 245 kV, or no Um is stated, check with us.

Nominal electrical stress

The electrical stress calculated at U0 using nominal dimensions, expressed in kV/mm (IEC 62067:2022, 3.3.2; the equations are in Clause 6, item n)). It decides whether a prequalification test is needed under IEC 60840: as amended in 2023, that standard requires one for cable systems whose calculated nominal stress exceeds 8.0 kV/mm at the conductor screen and/or 4.0 kV/mm at the insulation screen, with three exceptions.

Prequalification test

A long-term test of a complete cable system, made before that type of system is supplied on a general commercial basis (IEC 62067:2022, 3.2.4). IEC 62067 introduced it in its first edition on CIGRE’s advice, as a long-term accelerated ageing test on the complete system of cable, joints and terminations. An extension of prequalification (EQ, 3.2.5) takes an already prequalified cable system into account and needs roughly a quarter of the time of a full PQ test.

IEC 60840 introduced its PQ procedure in the fourth edition (2011), for cables with high electrical stresses at the conductor screen and/or insulation screen. Under its 2023 amendment, passing a PQ test covers the manufacturer for cable systems of the same family at the same or a lower rated voltage, provided the calculated stress at the insulation screen does not exceed that of the tested system (see nominal electrical stress). Utilities can make it a precondition: IPTO’s TD-102/3 does not accept a 400 kV cable whose manufacturer cannot submit a PQ certificate to clause 13 of IEC 62067.

A PQ test is made on a cable system, not on a compound, and none of the Borlink data sheets mentions one. More: prequalification in IEC 60840 and IEC 62067.

Routine, sample and type tests

The three kinds of test that IEC 60840:2020 and IEC 62067:2022 define in almost the same words (3.2.1–3.2.3):

  • Routine test: the manufacturer tests every component it makes (each cable length or accessory) against the specified requirements.
  • Sample test: at a set frequency, the manufacturer tests samples of finished cable, or parts taken from a finished cable or accessory, to check the finished product against the requirements.
  • Type test: made before a type of cable system (in IEC 60840 also a cable or an accessory) is supplied on a general commercial basis, to demonstrate satisfactory performance characteristics for the intended application. It need not be repeated unless changes in the materials, design or type of manufacturing process might change the performance characteristics.

IPTO’s TD-102/3 calls for routine tests to clause 9, sample tests to clause 10 and type tests to clause 12 of IEC 62067. How the standards relate to the compounds we supply: quality and standards.

IEC 60840 and IEC 62067

The two IEC test standards for AC power cables with extruded insulation and their accessories, split at 150 kV:

  • IEC 60840:2020 (with Amendment 1:2023): power cable systems, cables alone and accessories alone, for fixed installations and rated voltages above 30 kV (Um = 36 kV) up to and including 150 kV (Um = 170 kV); single-core and individually screened three-core cables.
  • IEC 62067:2022: power cable systems, cables with extruded insulation and their accessories, for fixed installations and rated voltages above 150 kV (Um = 170 kV) up to and including 500 kV (Um = 550 kV); single-core cables.

Both exclude special cables such as submarine cables, and transition joints to paper-insulated cables. On the current Borlink data sheets, the HV insulation grades (LE4244S, LS4201S) list both standards. The EHV insulation grades and both AC screen grades (LE0592S, LE0500) list IEC 62067, and each AC sheet notes that some standards may cover wider voltage ranges than its stated application. The standards set tests for cable systems, cables and accessories rather than compounds, and the Borealis sheets leave suitability testing to the customer. Compared in full: IEC 60840 vs IEC 62067.