How to choose a tackifier: a guide by polymer type
Start from the polymer. Match the resin’s polarity to the polymer, or to the block of it you want to modify, then set the softening point for the working temperature, and finally decide how much color and stability the job needs. Hydrocarbon, rosin and terpene resins each cover part of that map, and the table further down gives starting points by polymer type.
Why compatibility comes first
A tackifier is a low molecular weight resin added to raise tack, usually with a softening point above room temperature. Hot melts generally carry up to about 40%. Kraton calls compatibility with the adhesive polymer a crucial factor in viscoelastic properties, so the first question is whether the resin mixes.
Chemistry decides most of that. In a hydrocarbon resin, the balance of aliphatic and aromatic structure sets where it fits. Synthomer data sheets describe partially hydrogenated resins, with a balance of cycloaliphatic and aromatic structure, as reaching a breadth of compatibility that a purely aromatic or aliphatic resin cannot. Rosin esters also mix widely: Kraton lists high and low VA EVA, acrylics, SBR, SIS and SBS.
Kraton uses the Hildebrand solubility parameter as an estimate, since materials with similar values are likely to mix. Even so, a certain amount of incompatibility can give useful properties, so the parameter is a guide and not a rule.
Block copolymers add a second decision, because the resin can go to either block. In a styrenic block copolymer, a midblock tackifier such as a partially hydrogenated aliphatic resin adds tack. A pure monomer aromatic resin associates with the styrene endblocks and raises room-temperature cohesion. AMS resins, for example, are used to modify the styrene endblocks.
How the resin types compare
| Type | Raw material | Polarity | Color and stability |
|---|---|---|---|
| C5 | Petrochemical C5 monomers | Low | Light yellow, not hydrogenated |
| C9 | Petrochemical C9 aromatic monomers | Aromatic, higher | Darker |
| C5/C9 | Mixed aliphatic and aromatic monomers | Set by the aromatic share | Depends on the recipe |
| Pure monomer | Styrene, AMS | Aromatic | Water-white to very light; good oxidative stability |
| Hydrogenated | Aliphatic or aromatic resin, then hydrogenated | Low if fully hydrogenated; partial hydrogenation keeps some aromatic character | Low color; better heat, oxidation and UV resistance |
| Rosin esters | Pine rosin | Broad compatibility, from EVA to acrylics | Varies; stabilized and hydrogenated types improve it |
| Polyterpene | Turpentine | Low | Light color |
| Terpene phenolic | Terpene and phenol | Low to high, by hydroxyl level | Light to medium color |
More detail is in C5 vs C9, hydrogenated hydrocarbon resins, pure monomer resins, the rosin esters guide and terpene resins.
Decision guide by polymer
Use this as a starting list. The hydrocarbon and rosin entries follow the compatibility notes in Synthomer data sheets and Neville’s compatibility tables, and the terpene and AMS entries follow Kraton’s descriptions.
| Polymer | Start with |
|---|---|
| SEBS, SEPS, polyolefins, APAO | Hydrogenated hydrocarbon resins; highly hydrogenated rosin ester for APAO; polyterpene for polyolefins |
| SIS, natural rubber, polyisoprene | C5; hydrogenated hydrocarbon resins; rosin resins; polyterpene and low-polarity terpene phenolic for SIS |
| SBS, SBR, polybutadiene | Aromatic-modified C5; pure monomer; C9; rosin resins; low-polarity terpene phenolic for SBS |
| EVA under 30% VA | C5 and aromatic-modified C5; pure monomer; C9; rosin resins; terpene phenolic |
| EVA over 30% VA | Partially hydrogenated resins; rosin resins; high-hydroxyl terpene phenolic and AMS phenolic |
| Acrylics, polychloroprene, nitrile | Pure monomer; C9; rosin resins; low-polarity terpene phenolic for acrylic PSA |
| Styrene endblocks of SBC, polystyrene | Pure monomer; AMS; C9 |
Some grades state their target directly:
- Regalrez 1094 is listed for EVA and block copolymer hot melts.
- Regalite S7125 is listed for APAO and high-temperature hot melts.
- Wingtack 95 is described for SIS, natural rubber and other low-polarity elastomers.
- Cellolyn 21-E is listed for acrylic tapes and labels used in freezer conditions.
- Waterborne systems have their own option: AQUATAC tackifier dispersions for natural rubber, C-SBR, SBR, polychloroprene and acrylic latices.
Softening point and Tg
Softening point and Tg usually rise together. Across Kraton’s SYLVARES 1095 to 1160 terpene phenolics, Tg goes from 40 °C at a softening point of 96 °C on SYLVARES 1095 to 106 °C at 160 °C on SYLVARES 1160.
Higher-softening resins move heat resistance up. Cray Valley describes its higher-softening aromatic grades, Norsolene S-155 in particular, as raising the heat resistance of block copolymer PSA. Low-softening and liquid resins pull the other way: liquid Wingtack 10 is used to help low-temperature performance.
Softening point is the temperature at which a material passes a set, arbitrary softness, so compare figures only within one method. For resins that is usually ring and ball, ASTM E28. Pair the resin with a polymer of the right flow too. In EVA, that means VA content and melt index.
Color and stability
Hydrogenation lowers color and improves resistance to heat, oxidation and UV. Fully hydrogenated resins are non-polar. Partial hydrogenation keeps a balance of cycloaliphatic and aromatic structure, so the resin stays low in color and works with more polymers. Among rosin resins, stabilized and hydrogenated types are more stable than plain ones.
Color matters where the adhesive shows. Compare like with like: Gardner, yellowness index and Hazen are different scales, and data sheets read color either neat or in 50% toluene. Reading tackifier data covers these scales and the cloud points used to judge polarity.
Trial blends, grades and inquiry
No table replaces a trial. A workable order is:
- Write down the polymer, substrate, application method and service temperature.
- Pick two or three resin types from the table above.
- Blend at the target ratio and check that the blend stays clear and uniform.
- Test tack, peel and heat resistance on the real substrate.
For formula structure, see hot-melt adhesive basics and pressure-sensitive adhesive basics, or the hot-melt and PSA application pages. Values here are typical and are not specifications. We supply these grades. Send us your polymer and target softening point, and we will reply with grades to try.
References
- PDF · Kraton: Tackifiers for adhesives brochure · Hildebrand solubility parameter, useful incompatibility, terpene and AMS grades
- BRAND · Kraton: tackifiers for adhesives · Rosin ester, AMS, polyterpene and terpene phenolic compatibility
- PDF · Synthomer: REGALITE R1100 data sheet · Polymers listed for a fully hydrogenated resin
- PDF · Synthomer: REGALREZ 6108 data sheet · Partial hydrogenation, breadth of compatibility, EVA limit
- PDF · Synthomer: REGALITE C6100 data sheet · Midblock tackifier for block copolymers
- PDF · Synthomer: PICCOTAC 1095 data sheet · Polymers listed for an aliphatic C5
- PDF · Synthomer: PICCOTAC 8095 data sheet · Polymers listed for an aromatic-modified C5
- PDF · Synthomer: KRISTALEX 3100 data sheet · Pure monomer resin, styrene endblocks, polar rubbers, EVA limit
- PDF · Synthomer: ENDEX 160 data sheet · Endblock resin, polystyrene compatibility
- PDF · Synthomer: FORAL 85-E data sheet · Hydrogenated rosin ester, oxidation resistance, compatibility
- WIKI · Softening point · Definition and test methods
- WIKI · Tackifier · Definition and main classes
- WIKI · Hot-melt adhesive · Tackifier loading