EVA vinyl acetate content and melt index: how to choose
Vinyl acetate (VA) content sets EVA’s crystallinity, melting point, softness and polarity. Melt index (MI) sets how easily it flows, and with that its strength and cohesion. For a hot melt, choose VA first from the substrate and temperature range, then choose MI for the application viscosity and the bond strength you need. The figures below are typical values for ExxonMobil Escorene Ultra grades, used only as examples.
What VA content changes
EVA is a copolymer of ethylene and vinyl acetate, usually with 1 to 40 wt% VA. Up to about 4% it behaves like a modified low-density polyethylene. From about 4% to 30% it behaves more like a rubber or plasticized PVC. Hot-melt grades sit in the middle and upper part of the scale. VA units break up the ethylene crystals, so crystallinity and melting point fall as VA rises and clarity improves. Tensile strength falls too, as the tables below show.
VA also moves the polymer toward the polar side. In hot melts, more ethylene favors bonding to non-polar surfaces such as polyethylene. More VA brings flexibility, adhesion, hot tack and better low-temperature performance, at the cost of solvent resistance.
Three groups of Escorene Ultra grades at similar MI show the effect:
| Grade | VA, wt% | MI, g/10 min | Melting point, °C | Tensile strength, MPa | Elongation, % |
|---|---|---|---|---|---|
| UL 15019CC | 19 | 150 | 83 | 4.9 | 650 |
| UL 15028CC | 27.5 | 150 | 69 | 3.6 | 830 |
| AD 0428EM1 | 27.5 | 400 | 71 | 3 | 700 |
| AD 0433EH2 | 33 | 400 | 59 | 1.7 | 710 |
| UL 04028CC | 27.5 | 41 | 71 | 6.5 | 720 |
| UL 04533EH2 | 33 | 45 | 62 | >4.0 | >750 |
| UL 05540EH2 | 39 | 60 | 48 | >1.8 | >750 |
At MI 150, going from 19 to 27.5 wt% VA takes the melting point from 83 to 69 °C and tensile strength from 4.9 to 3.6 MPa, while elongation rises from 650% to 830%. The other two groups show the same fall in melting point and strength.
Melting point also bears on service temperature. A general reference limits EVA adhesives to use below 60–80 °C and notes low creep resistance under load. On the Escorene Ultra list, melting point runs from 48 °C for UL 05540EH2 to 87 °C for UL 00218CC3, so check a high-VA grade against the end-use temperature.
What melt index changes
MI is the mass of polymer, in grams, pushed through a standard die in 10 minutes at a set temperature and load, by ASTM D1238 or ISO 1133. ExxonMobil’s EVA data sheet uses 190 °C and 2.16 kg. A high MI means lower molecular weight and lower melt viscosity. It is a single low-shear reading, so two resins with the same MI can process differently.
In a hot melt, lower molecular weight chains wet better and adhere better to porous surfaces, while higher molecular weight helps cohesion at elevated temperature and low-temperature behavior.
These Escorene Ultra grades hold VA near 27.5 wt% and raise the flow:
| Grade | VA, wt% | Flow | Melting point, °C | Tensile strength, MPa |
|---|---|---|---|---|
| UL 00728 | 27.5 | MI 7 | 73 | 17 |
| UL 02528 | 27.5 | MI 25 | 71 | >6.5 |
| UL 04028CC | 27.5 | MI 41 | 71 | 6.5 |
| UL 15028CC | 27.5 | MI 150 | 69 | 3.6 |
| AD 0428EM1 | 27.5 | MI 400 | 71 | 3 |
| UL 8705 | 27.6 | 9300 mPa.s Brookfield, 190 °C | 71 | 2 |
| AD 2528 | 27.6 | 3200 mPa.s Brookfield, 190 °C | 74 | 2 |
Across this series the melting point stays between 69 and 74 °C, so VA and not flow is what sets it. Tensile strength falls from 17 to 2 MPa. The last two grades are listed by Brookfield viscosity instead of MI, and lower viscosity there means easier flow.
EVA in a hot melt
One published example of an EVA hot melt is 30–40% EVA for strength and toughness, 30–40% tackifier for wetting and tack, 20–30% wax for viscosity, setting speed and cost, and 0.5–1.0% stabilizer. Adhesive-grade EVA usually holds 14–35% VA, and one reference gives about 18–29%. The Escorene Ultra list spans 18 to 39 wt%, and ExxonMobil names packaging, bookbinding, woodworking, assembly, carpet backing, wax blending and road marking as uses. See hot-melt adhesives, road marking paint and hot-melt formulation basics.
VA also steers the resin choice. Synthomer data sheets show how far each resin type reaches:
- Low VA: C5 resins.
- Up to 30% VA: pure monomer resins.
- Up to 40% VA: partially hydrogenated grades among the hydrogenated resins.
Rosin esters are listed for both high and low VA EVA, terpene phenolic resins are a common EVA tackifier, and some C9 grades are listed for EVA hot melts. ExxonMobil’s data sheet for a high-flow grade near 28% VA states very good compatibility with hydrocarbon and natural tackifiers and most waxes. The full table is in how to choose a tackifier.
EVA with wax
Wax lowers viscosity and changes setting speed, and hot melt formulas usually use paraffin types. How well wax and EVA mix depends on the melting points of the two and on VA content. Public data give no single cut-off, only specific cases:
- EVA with 28 wt% VA and paraffin formed stable, homogeneous blends in most conditions in a University of Birmingham study. Viscosity rose strongly with EVA content, and the brittle wax turned flexible.
- EVA with 20% VA was miscible in microcrystalline wax up to at least 30% in a viscosity study.
- A patent notes that EVA wax blends are common in hot melts and in wax coatings for paper boxes.
The first two studies concern ceramic binders, not adhesives, so treat them as pointers. Check your own wax at your application temperature.
Narrowing the choice
The two tables above are the two levers. At similar VA, MI changes flow with little effect on melting point. At similar flow, VA changes melting point, strength and polarity.
- Set VA from the substrate and temperature. Higher VA suits flexibility, adhesion, hot tack and low-temperature use. Lower VA keeps a higher melting point and more strength at the same flow.
- Set MI from the application. Pick for the viscosity your equipment needs, then check the cohesion and strength.
- Check resin and wax. Use VA to select the tackifier, and blend with your wax.
- Run a trial on the real substrate.
If EVA does not fit, the same polyolefin section lists EnBA and EMA copolymers, Vistamaxx polymers and APAO.
Grades and inquiry
All 28 Escorene Ultra grades are on the EVA page and the ExxonMobil brand page. Values here are typical and are not specifications. We supply these grades. Send us your VA range, MI or viscosity target and end use, and we will reply with matching grades.
References
- PDF · ExxonMobil EVA 150028 product datasheet · Tackifier and wax compatibility, MI test condition
- PDF · Synthomer: PICCOTAC 1095 data sheet · Aliphatic C5, low-VA EVA
- PDF · Synthomer: KRISTALEX 3100 data sheet · Pure monomer resin, EVA up to 30% VA
- PDF · Synthomer: REGALREZ 6108 data sheet · Partially hydrogenated resin, EVA up to 40% VA
- BRAND · Kraton: tackifiers for adhesives · Rosin esters with high and low VA EVA
- PAPER · Investigation into paraffin wax and ethylene vinyl acetate blends · Standring, Blackburn, Wilson, University of Birmingham, 2016
- PAPER · Binder formulation in EVA-wax system for fused deposition of ceramics · Pekin, Zangvil, Ellingson, 1998; VA, crystallinity and wax compatibility
- PATENT · US 7,135,508, Coatings and films derived from clay/wax nanocomposites · EVA with 28 wt% VA and paraffin; uses of EVA wax blends
- WIKI · Hot-melt adhesive · EVA grades, example formula, effects of VA and molecular weight
- WIKI · Melt flow index · Definition, link to molecular weight, limits of the test