Hot-melt adhesive formulation basics: polymer, tackifier, wax
A hot-melt adhesive is a thermoplastic that is applied molten and sets as it cools. Most formulas have four working parts: a base polymer for strength and cohesion, a tackifier for wetting and tack, a wax that thins the melt and speeds setting, and an antioxidant that keeps the melt stable. The polymer family shapes the rest of the formula, so this guide explains each part and then goes through EVA, APAO and styrenic block copolymer systems.
Grade figures come from producers’ data and are typical values, not specifications.
What each part does
| Part | Job in the formula | Common materials |
|---|---|---|
| Base polymer | Strength, toughness and cohesion | EVA, APAO and other polyolefins, SBC |
| Tackifier | Better wetting and tack | Rosin esters, terpene and terpene phenolic resins, C5, C9, C5/C9 and hydrogenated hydrocarbon resins |
| Wax | Lower melt viscosity, faster setting | Paraffin, microcrystalline and oxidized Fischer-Tropsch waxes |
| Plasticizer (optional) | Softer adhesive, lower melt viscosity | Paraffin oils, polyisobutylene |
| Antioxidant | Protection during compounding, in the melt and in service | Hindered phenols, phosphites |
Two figures give a sense of scale. Tackifiers can reach about 40% of the formula and are often the largest share of its weight and cost, while antioxidants go in at under 1%. The formula is set so that its glass transition sits below the lowest service temperature, because the adhesive turns brittle below it.
EVA systems
EVA is a low-cost polymer and the most common base for glue sticks, and nearly half of EVA hot melts go into packaging. Its vinyl acetate (VA) content steers adhesion: more ethylene favors non-polar surfaces such as polyethylene, and more VA favors polar surfaces such as paper. The article on EVA vinyl acetate content covers this in detail.
VA also moves the melting point. In the ExxonMobil Escorene Ultra series, UL 15019CC and UL 15028CC share a melt index of 150 g/10 min, with comonomer contents of 19 and 27.5 wt% and melting points of 83 and 69 °C. Melt index runs roughly inverse to molecular weight: a high value is easy to apply but gives weaker mechanical properties.
EVA is a polar polymer, so resins with some polarity are the usual partners. Kraton lists its rosin esters as compatible with both high and low VA EVA, terpene phenolic resins are often used with EVA, and Cray Valley describes aromatic-modified resins such as Norsolene A-100 for EVA hot melts.
One published EVA hot-melt example is 30–40% EVA, 30–40% tackifier, 20–30% wax (usually paraffin-based) and 0.5–1.0% stabilizers, from the Wikipedia article on hot-melt adhesives. It shows proportions only and is not a starting formula. The same source notes EVA’s limits: low creep resistance under load, and use limited to below 60–80 °C.
APAO and other polyolefin systems
Amorphous polyolefins (APO or APAO) are tacky, soft and flexible. Compared with similar EVA adhesives they tend to have lower melt viscosity, better adhesion, longer open time and slower set. Some can be used alone, but they are often compounded with tackifiers, waxes and plasticizers such as mineral oil or polybutene oil (see the polyisobutylene guide). Their cohesion is relatively low, so cohesive failure is a common failure mode.
Synthomer Eastoflex shows how polymer type changes the numbers:
| Grade | Polymer type | Viscosity at 190 °C, mPa·s | R&B softening point, °C | Tg, °C | Needle penetration, dmm |
|---|---|---|---|---|---|
| P1010PL | Polypropylene homopolymer | 1000 | 155 | -10 | 18 |
| M1030PL | Polypropylene / propylene-ethylene copolymer blend | 3000 | 155 | -12 | 20 |
| E1060PL | Propylene-ethylene copolymer | 5700 | 140 | -20 | 35 |
Vistamaxx polymers are a related route. ExxonMobil describes its low-viscosity hot-melt type as a propylene elastomer with isotactic propylene units and randomly distributed ethylene, made with a metallocene catalyst. Vistamaxx 8880 has a viscosity of 1200 cP at 190 °C. Metallocene polyolefins generally have a narrow molecular weight distribution and a narrow melting range.
SBC systems
SBS, SIS and SEBS usually have an A-B-A structure: an elastic rubber block between two rigid endblocks. The endblocks separate into their own phase and hold the rubber together, so no extra cross-linking is needed. These adhesives are often pressure-sensitive and keep their tack after cooling, a topic covered in pressure-sensitive adhesive basics. In broad terms, SBS is used for high strength, SIS for low viscosity and high tack, and SEBS for low-tack nonwoven work.
Because the polymer has two phases, a resin’s effect depends on where it goes:
- Midblock resins: aliphatic resins such as C5, rosin esters, polyterpenes and terpene phenolics. They improve adhesion, processing and pressure-sensitive properties.
- Endblock resins: indene-coumarone, alpha-methylstyrene and other aromatic types, including many pure monomer resins. They improve adhesion and alter viscosity.
Plasticizing oils lower cost, melt viscosity and hardness, and improve tack and low-temperature flexibility. Stability needs more care with unhydrogenated polymers: SIS can undergo chain scission during long hot mixing, which lowers viscosity and performance. SEBS has a saturated midblock and resists heat and oxygen better. Hydrogenated resins such as Regalrez 1094, listed for EVA and block copolymer hot melts, are common where light color and stability matter.
Wax and antioxidant
Wax lowers melt viscosity and controls open time and set speed. A patent on hot-melt waxes (US 6,890,982) notes that formulators keep the wax level as low as those targets allow. Paraffin-based waxes are usual in EVA formulas. Several series in the grade tables list wax blending among their uses, including Escorez 1000 and Escorene Ultra EVA.
Antioxidants matter because a hot melt can stay molten for long periods before it is applied. EVA degrades mainly by losing acetic acid and by oxidation, and additives with unsaturated bonds, such as rosin-based resins, are prone to autoxidation. Hindered phenols and phosphites are the common choices. BASF’s Irganox B 225 data sheet shows the usual logic: the phosphite protects during processing, and the hindered phenol gives long-term thermal stability. NEVASTAIN 21 from the antioxidant list is a non-staining Neville product for EVA hot melts and SIS or SBS pressure-sensitive adhesives.
What to check in a trial
- Melt viscosity. It governs spreading and wetting, and it falls as temperature rises. Brookfield viscosity is the usual number, with methods such as ASTM D3236.
- Softening point. See the glossary entry and how to read tackifier data.
- Open time and set time. Open time is the working time while the surface still has enough tack. Set time is the time to reach an acceptable bond.
- Pot life stability. This is the melt’s resistance to decomposing and charring during long periods at temperature.
- Service temperature. Check both ends of the range on the real substrate.
Grades and inquiry
The hot-melt adhesives page lists materials for this use, and choosing a tackifier goes deeper on resins. We supply these grades. Tell us your polymer system, application temperature and substrates, and we will reply with suitable options.
References
- ENCYCLOPEDIA · Hot-melt adhesive · Wikipedia; components, base polymers, example EVA composition, open time and pot life
- ENCYCLOPEDIA · Tackifier · Wikipedia; molecular weight, softening and share of the formula
- ENCYCLOPEDIA · Melt flow index · Wikipedia; relation to viscosity and molecular weight
- PATENT · US 6,890,982 B2, Wax for hot melt adhesive applications · Background on polymer, tackifier and wax
- TRADE · Rubber-based hot-melt pressure-sensitive adhesives · Adhesives & Sealants Industry; SIS heat stability
- TRADE · Hydrogenated styrenic block copolymers for adhesives and sealants · Adhesives & Sealants Industry; SEBS stability and hydrogenated resins
- TRADE · Low-molecular-weight polyolefins for hot-melt adhesives · Adhesives & Sealants Industry; polymer, tackifier, diluent and additive
- BRAND · VESTOPLAST brochure · Evonik; APAO as a hot-melt raw material
- BRAND · Vistamaxx performance polymer 8580 data sheet · ExxonMobil; propylene elastomer description
- BRAND · Irganox B 225 technical data sheet · BASF; phosphite and hindered phenol roles