Hydrogenated hydrocarbon resins: color, stability, hot melts
Choose a hydrogenated petroleum resin when a hot melt must look clear or stay molten for long periods. Hydrogenation adds hydrogen to the double bonds left in a hydrocarbon resin, so the resin comes out paler and more resistant to heat, oxidation and UV light. The further hydrogenation goes, the more aliphatic the resin behaves, and a partly hydrogenated resin keeps some aromatic character. So let the base polymer decide between full and partial hydrogenation.
Grade figures below are typical values from the tables on this site, not specifications. The exception is Lanzhou Petrochemical: its figures are limits and ranges, not typical values. Each example stays within one brand, because brands use different test methods and color scales.
Why hydrocarbon resins are hydrogenated
A polymerized resin still carries unsaturated bonds, and they cost it color and stability. A Royal Society Open Science paper describes C9 resin as yellow or amber, with malodor, poor thermal stability and poor oxidation resistance. An Exxon patent says much the same of thermally polymerized resins: rather dark, and thermally and oxidatively unstable.
Bromine number, the grams of bromine absorbed by 100 g of sample, falls as double bonds are removed, so it shows how much unsaturation is left. That Exxon patent reports about zero after hydrogenation.
The base resin can be aliphatic or aromatic: see C5 vs C9 hydrocarbon resins.
Color and stability
Hydrogenation can take a hydrocarbon resin to a very pale or water-white color, and water-clear hot melts rely on raw materials such as hydrogenated tackifiers.
ExxonMobil tables show the range of color. Escorez 1304 in the aliphatic 1000 series has a softening point of 99.7 °C and a yellowness index of 29. Escorez 5300, a water-white hydrogenated cycloaliphatic resin, softens at 105 °C with a yellowness index of ≤1. Both are measured at 50% in toluene. The two series are built differently, so this gap does not measure hydrogenation alone.
Lanzhou Petrochemical grades its hydrogenated C5 resins by color and sets a bromine limit for the palest ones: the paler the grade, the lower the limit.
| Grade | Softening point, °C | Color (50% toluene) | Bromine number, g/100 g, max |
|---|---|---|---|
| LH100-0 | 96–105 | YI <3.50 | 1 |
| LH100-1 | 96–105 | YI 3.50–9.49 | 2 |
| LH100-2 | 96–105 | Gardner 1.1–2.0 | 3 |
| LH100-3 | 96–105 | Gardner 2.1–3.0 | 5 |
Stability follows the same logic. With fewer double bonds there is less for heat and oxygen to attack. An ExxonMobil packaging brochure makes the practical point: hydrogenated tackifiers have higher thermal stability than non-hydrogenated resin, which keeps color consistent through production, reduces char and gel, and helps hold adhesive viscosity. An Exxon patent on liquid aliphatic resins also reports better thermal and UV stability after hydrogenation.
Degree of hydrogenation
Hydrogenation does not have to run to completion. Synthomer makes partially hydrogenated Regalrez grades that stay pale and keep a balance of cycloaliphatic and aromatic structure, so color and compatibility can be set separately.
To compare grades on degree of hydrogenation, use MMAP, DACP and bromine number, not the label. MMAP falls as aromatic content rises and DACP falls as polarity rises, so high values of both point to aliphatic character and can indicate how far hydrogenation has gone. Synthomer Regalrez grades spread widely while color barely moves:
| Grade | Softening point, °C | Color YID | DACP, °C | MMAP, °C |
|---|---|---|---|---|
| Regalrez 1094 | 95 | 2 | 59 | 84 |
| Regalrez 6108 | 108 | 3 | 25 | 53 |
| Regalrez 3102 | 102 | 3 | -15 | 24 |
Regalrez 1094 sits at the aliphatic end and 3102 keeps far more aromatic character, yet all three are pale. See how to read tackifier data.
The polymer has to accept the resin, and Synthomer’s data sheets for these two grades show the split:
- Regalrez 1094, fully hydrogenated: polyethylene, polypropylene, natural and synthetic rubbers, EPDM, butyl rubber, APAO, waxes, and the midblock of SIS, SEPS and SEBS.
- Regalrez 3102, partially hydrogenated: natural rubber, SBR, polychloroprene, the midblock of SBS, SIS, SIBS and SEBS, and the styrene end blocks of block copolymers.
Aromatic content is a trade-off, as a published study of hydrogenated DCPD resins shows. All the resins tackified SIS. In SBS, room-temperature loop tack came only from those with aromatic H above 3 wt% and/or a softening point below 110 °C. At equal softening point, more aromatic content raised peel and loop tack, while high aromatic content lowered high-temperature resistance.
What the hydrogenated ranges are
- ExxonMobil Escorez 5000: the 5300 series is water-white hydrogenated cycloaliphatic, 5400 is light-color hydrogenated cycloaliphatic, and 5600 is light-color hydrogenated aromatic-modified cycloaliphatic. The 5000 series lists nonwovens, packaging, bookbinding, woodworking, assembly, sealants, tapes, labels and wax blending.
- Synthomer: MMAP shows how far each hydrogenated range spreads. Eastotac holds 78 to 85 °C across softening points from 100 to 142 °C, so it stays near the aliphatic end. Regalite runs from 55 to 86 °C. Regalrez runs from 24 to 109 °C. Regalrez 3102 and 6108 sit below every Regalite grade, so start with those when the polymer needs some aromatic character. Plastolyn R1140 is listed for plastics modification.
- Lanzhou Petrochemical LH: made from the C5 fraction of ethylene cracking, then hydrogenated, in 90, 100 and 110 softening point bands, and listed for hot melts and pressure-sensitive adhesives, among other uses.
Use in hot melts
Tackifiers can reach about 40% of a hot melt’s mass, so the resin has a large effect on the whole adhesive. Hot melts often sit molten in a tank before application, and stability there, called pot life, is where a hydrogenated resin helps: it holds color and viscosity better and is less prone to char. See hot-melt adhesive formulation basics for how resin, polymer and wax work together.
Choose first by base polymer, then by softening point:
- EVA: resin polarity must match the vinyl acetate content. See EVA vinyl acetate content and the EVA grades.
- SEBS and SEPS: fully hydrogenated, low-polarity resins work in the midblock. See the SEBS grades.
- APAO: Regalite S7125 is listed for hot melts based on APAO and for high-temperature use.
Within a series, a higher softening point usually means a higher Tg and a higher melt viscosity. It generally supports heat resistance, and a lower one gives easier flow. In ExxonMobil’s 5300 series, Escorez 5380 softens at 86.2 °C with a Tg of 36 °C, and Escorez 5340 at 139.5 °C with a Tg of 86 °C.
In Eastotac, listed uses narrow as softening point rises. At 100 °C, Eastotac H-100W is listed for packaging, nonwovens, assembly, glue sticks and hot-melt PSA. At 130 °C, Eastotac H-130R is listed for packaging and assembly only. So in that range use the lower grades for PSA, nonwovens and glue sticks, and go higher when heat resistance calls for it.
Choosing and asking for a grade
Start from the polymer and how long the adhesive stays hot, then narrow by color, softening point and cloud points. Test the short list in your own formulation, including an aging run at application temperature. We supply these grades: see the hot-melt adhesives page and send us your polymer, softening point and volume.
References
- BRAND · Polymers and tackifiers for hot melt adhesives in packaging · ExxonMobil brochure; effect of hydrogenation on heat stability
- BRAND · Regalrez 1094 data sheet · Synthomer; fully hydrogenated grade, compatibility
- BRAND · Regalrez 3102 data sheet · Synthomer; partially hydrogenated grade, compatibility
- PAPER · A Ni-based catalyst … for C9 petroleum resin (C9 PR) hydrogenation · Chen et al., Royal Society Open Science, 2018; properties of C9 resin
- PATENT · US 4,629,766, Production of hydrofined hydrocarbon resins · Exxon; color, stability, bromine number
- PATENT · US 4,916,192, Hydrogenated liquid aliphatic hydrocarbon resins · Exxon; thermal and UV stability after hydrogenation
- PATENT · US 5,213,439, Process for marking a pavement · Shell; what MMAP and DACP indicate
- TRADE · Hydrogenated DCPD-Based Resins for SBC-Based Hot-Melt PSAs · Lee, Adhesives & Sealants Industry, 2012; SIS and SBS tack study
- ENCYCLOPEDIA · Petroleum resin · Hydrogenation and water-white resins
- ENCYCLOPEDIA · Bromine number · Definition and units
- ENCYCLOPEDIA · Hot-melt adhesive · Tackifier share, pot life, color