SBS modified asphalt: how it works, linear vs radial, grades

· Updated · Application

SBS modified asphalt, also called SBS modified bitumen, is asphalt binder with styrene-butadiene-styrene block copolymer blended in: a polymer modified bitumen (PMB) used for paving and roofing. SBS makes asphalt more elastic. The polymer swells in the light fractions of the asphalt and forms a network, which helps the binder resist rutting in heat and cracking at intermediate temperatures. Choose radial SBS when softening point and rutting resistance come first and linear when you need lower viscosity, then narrow the grade by your base asphalt, dose and mixing equipment.

At a glance

Point Figure Source
SBS in a conventional modified paving binder Roughly 3% polymer FHWA case study
SBS in highly modified asphalt (HiMA) 7 to 8% FHWA case study
Kraton’s range for paving 2 to 8 wt% SBS Kraton
One roofing formula 8.72 wt% SBS, linear and radial blended Tremco patent
Hot storage of the binder Little change up to 150 °C, fast loss from 180 °C Singh and co-workers (2018); CETRA 2026 paper
Linear or radial Radial raises softening point more; linear keeps viscosity lower Comparison below

How SBS works in asphalt

Kraton says the effect of SBS depends on polymer content, polymer type and the formulation process, and the structure in the binder shows why. See also the asphalt modification page.

SBS swells into a two-phase structure of swollen polymer and asphalt. With longer shear, Li and co-workers (2026) saw fewer, larger particles under a fluorescence microscope and a sharp rise in viscosity, so keep shear time equal when you compare binders. At higher polymer content, an FHWA case study says the phases reverse, leaving asphalt dispersed in swollen polymer, and the binder behaves more like rubber.

Paving

Set the dose first. The FHWA study puts conventional modified binders at roughly 3% polymer and highly modified asphalt (HiMA) at 7 to 8%, and Kraton’s own range for both together is 2 to 8 wt% SBS. Florida first adopted HiMA for severe rutting in high-stress locations such as truck weigh stations and busy intersections.

More polymer is not free. A 2026 review in the Journal of Testing and Evaluation links phase inversion at high dose with problems in blending, compatibility, workability and long-term storage stability. Recheck blending and storage before you raise the dose.

Roofing

A membrane supplier’s training course and a roofing patent point to the same needs: a compound that stays elastic and flexible in the cold, survives hot blending, and reaches its softening point without too much viscosity. The course quotes cold flexibility below -20 °F (about -29 °C), which is one supplier’s figure, and warns that too much filler reduces elastic properties. It puts blending at about 400 °F (204 °C), and too much mixing time or heat can break the compound down. For the viscosity balance, a Tremco patent on roofing impregnating asphalt uses 8.72 wt% SBS in its example, split between linear and radial polymer: the next section gives its figures.

Standards: an Asphalt Roofing Manufacturers Association product declaration says membranes comply with one or more of ASTM D6162, D6163, D6164 and CSA A123.23; in China, GB/T 18242-2025 for elastomer and plastomer modified bitumen waterproofing sheets took effect on 1 May 2026.

Linear or radial

Property Linear SBS Radial SBS
Softening point Smaller rise Larger rise
Rutting resistance Lower at the same dose Higher; studies differ on how the gap moves with dose
Form in asphalt Disperses as globules, improves ductility Tends toward a crosslinked network
Viscosity Lower Higher

Sources: Liang and co-workers (2016) for softening point and form, Huang and co-workers (2015) for rutting.

The studies disagree on dose. Huang found the rutting gap narrowing as SBS content rose, while Zhu and co-workers (2024), comparing diblock, linear and radial SBS at 3% and 6%, point the other way: the effects of structure were limited at low polymer content and larger at high content. The two studies measured different things, so do not assume the gap between types shrinks or grows with dose.

Viscosity is the price of radial structure. In the Tremco roofing formula, going from all linear to all radial raised softening point from 247.3 to 258.7 °F (about 120 to 126 °C) and initial viscosity at 375 °F from 15,520 to 30,080 cps, so the patent blends the two. Kraton’s typical data agree: at 25 wt% in solution, linear D1101 is 4000 mPa·s and radial D1184 is above 20,000 mPa·s, at the same 31/69 styrene/rubber ratio.

Zhu and co-workers also report that structure affects storage stability, but we found no consistent rule for which structure stores better.

So start from radial if softening point and rutting resistance are the target, linear if viscosity is the limit, and consider a blend, as the Tremco roofing patent does, if you need both, then settle dose and storage in the grade trial below.

Storage and heat

In lab storage studies, binders changed little up to 150 °C and lost properties fast from 180 °C. Singh and co-workers (2018) saw no property loss in sealed tubes at 150 °C for up to 21 days, significant erosion within 3 days at 180 °C and above, and base asphalt values within a day at 210 °C. In a 2026 CETRA paper, storage at 120 and 150 °C made little difference over 14 days, while 180 °C cut elastic recovery by about 34% and 47% after 7 and 14 days. Low-vinyl SBS lost elastic recovery fastest, and high-vinyl types held up better. If binder must wait, hold it nearer 150 °C than 180 °C.

Do not judge segregation on softening point difference alone. Lin and co-workers (2012) tested eight commercial binders and concluded that a softening point difference of 2.5 °C or less is not enough on its own to judge storage stability. A 2024 study from the same group proposes phase particle size as a faster control.

What to look for in a grade

  • Structure. Kraton lists asphalt use for its D 1100 and 4100 series. Linear grades include D1101 and D1192; radial grades include D1184, D1191 and D1194. TSRC lists asphalt use for radial 2336A and 2411A, and linear 2518A / 2518ALD and 3201.
  • Styrene. The grades above all sit around 30%, so styrene alone will not separate them.
  • Diblock. Kraton says diblock helps balance viscosity and mixing in asphalt. D1192 is below 1%, and D1101 and D1184 are at 16%.
  • Viscosity and melt flow. Compare at the same concentration. TSRC does not quote all these grades at one, so its numbers are not always comparable.
  • Physical form. Grades come as porous pellet or powder. Check ash on powder: TSRC 2411AP lists 5 wt% against 0.5 for 2411A, and 2518AP / 2518APC lists 5 wt%. Ask which form suits your mixer.
  • Vinyl content. If binder sits hot for days, ask about it.
  • Ready modifiers. D3158 is a pre-compounded asphalt modifier in the SBC compounds range.

The base asphalt has the last word. Trial the shortlist at your real dose, temperature and shear time, and include a storage check.

Grades and inquiry

For saturated polymers see SBS vs SEBS, and for adhesives see SIS vs SBS in adhesives. For colored asphalt, hydrogenated C5 resins are listed for that use, and our hydrogenated resins article covers their color and stability. More grades are on the Kraton and TSRC brand pages. Grade figures are typical values, not specifications. We supply these grades: send us your asphalt source, target dose and paving or roofing use and we will suggest similar grades.